The development of thermonuclear experimental reactor (ITER), whose objective is to produce energy from nuclear fusion, has raised the study of Pb-Li eutectic alloys, as they have been selected for the manufacture of test blanket modules (TBM). However, during the manufacturing process of the Pb-Li alloys, thermal conditions used result in a loss of litium element, which inhibits the formation of eutectic structures. In this work we have done fusion of pure lead and lithium, evaluating different process parameters to obtain Pb-Li (17 at. %) eutectic alloys. The alloys manufactured were characterized by DSC, SEM-EDX and microhardness tests. From these studies we noted that the used of an induction reactor and the process parameters optimized to obtain Pb-Li alloy allow for completely eutectic ingots and high chemical homogeneity and microstructural.