Refrigerator glass shelves are manufactured by Insert Injection Molding. The current process of injection of glass into the mold induces movement of the core, on urethane springs. Defects in the product can result from too low a force being transmitted from the springs. To solve this problem, the force on the moving core and the injection molding pressure were subjected to numerical analysis. Based on this, the number of urethane springs as well as their hardness was changed to improve the situation. The number of springs was changed from 6 to 4. The diameter of the springs was increased from Ø75 to Ø100, and the hardness was increased from 70 (shore A) to 90 (shore A). These improvements caused the force on the molding core to increase by approximately 65,442 N. The proportion of defects decreased by 66%.